GR1 Titanium Chemical Composition and Material Properties
May 18, 2026
What Is GR1 Titanium?
GR1 (Grade 1, UNS R50250) is the softest and most ductile grade of commercially pure (CP) titanium. With a minimum titanium content of 99.5% and a maximum oxygen content of 0.18%, GR1 offers the highest formability of all CP grades while retaining titanium's characteristic corrosion resistance. It is used where deep drawing, severe forming or maximum ductility is required, for example in chemical processing, marine engineering and medical devices.
Chemical Composition Limits
| Element | Maximum Weight % |
|---|---|
| Titanium (Ti) | Balance (min 99.5%) |
| Iron (Fe) | 0.20 |
| Oxygen (O) | 0.18 |
| Carbon (C) | 0.08 |
| Nitrogen (N) | 0.03 |
| Hydrogen (H) | 0.015 |
Role of Each Element
Oxygen is the most important strengthener; at 0.18% max it keeps GR1 soft and ductile. Higher oxygen raises strength but reduces formability.
Nitrogen strengthens strongly but also reduces ductility and must be kept below 0.03%.
Hydrogen above 0.015% can cause embrittlement, especially in weldments, so it is strictly limited.
Iron is a common impurity that adds strength; the 0.20% maximum keeps the alloy soft.
Mechanical and Physical Properties
| Property | Value |
|---|---|
| Tensile strength, min | 240 MPa (35 ksi) |
| Yield strength (0.2% offset), min | 170 MPa (25 ksi) sheet per ASTM B265; 138 MPa (20 ksi) tube per ASTM B861 |
| Elongation, min | 24% |
| Density | 4.51 g/cm3 |
| Melting point | 1668 deg C |
| Thermal conductivity | 17 W/(m.K) |
| Coefficient of thermal expansion | 8.6 x 10-6 /K |
Heat Treatment
GR1 is normally used in the annealed condition. Annealing at 704-815 deg C optimizes toughness and ductility and is recommended after significant cold work or when maximum formability is required. Because GR1 cannot be strengthened by heat treatment, cold working is the only practical way to raise its strength.
Welding and Forming
GR1 welds readily when the molten and heat-affected zones are protected from air contamination. Argon shielding on both the face and root of the weld is essential to prevent oxygen and nitrogen pickup, which would embrittle the joint. The alloy is the best CP grade for cold forming: deep drawing, bending and flanging are performed without difficulty, and springback is low.
Applications
Chemical processing: corrosion-resistant piping, reactors, heat exchanger tubes and fittings.
Marine engineering: seawater piping, pump components and desalination equipment.
Medical devices: surgical instruments and implants per ASTM F67 Grade 1.
Deep-drawn parts: heat exchanger tube sheets, filter housings and containers.
Equivalent Standards
| Standard | Designation |
|---|---|
| UNS | R50250 |
| Werkstoff number | 3.7025 |
| ASTM pipe | B338 Grade 1 |
| ASTM seamless tube | B861 Grade 1 |
| ASTM welded tube | B862 Grade 1 |
| ASTM sheet/plate | B265 Grade 1 |
| Medical implant | ASTM F67 Grade 1 |
| ISO | 5832-2 Grade 1 |
| JIS | H4600 Class 1 |
| China | TA1 (GB/T 3620.1) |
GR1 vs GR2
The practical difference between GR1 and GR2 is oxygen content: GR1 limits oxygen to 0.18% and GR2 to 0.25%. This makes GR1 softer (yield about 170 MPa vs 275 MPa for sheet) and more ductile (24% vs 20% elongation). Selection is straightforward: choose GR1 when formability and deep drawing dominate, and GR2 when a balance of strength and cost is needed.
FAQ
What is the chemical composition of GR1 titanium?
GR1 is at least 99.5% titanium with maximums of 0.20% iron, 0.18% oxygen, 0.08% carbon, 0.03% nitrogen and 0.015% hydrogen.
What is the UNS number for GR1 titanium tube?
UNS R50250; the Werkstoff number is 3.7025, and medical grade is ASTM F67 Grade 1.
Why is GR1 more formable than other titanium grades?
Its very low oxygen content (0.18% max) keeps interstitial strengthening low, giving the highest ductility and lowest yield strength among CP grades.
Can GR1 titanium be welded?
Yes, with argon shielding on both sides to prevent oxidation and nitriding; the alloy has good weldability when contamination is avoided.
What is the annealing temperature for GR1 titanium?
Annealing at 704-815 deg C restores toughness and ductility and is recommended after heavy cold work.
What is the difference between GR1 and GR2 titanium?
GR1 has a lower oxygen limit (0.18% vs 0.25%), giving lower strength and higher ductility; GR2 offers higher strength at slightly lower formability and is the most common CP grade.