ASTM B338 Grade 7 Titanium Tube for Heat Exchanger and Condenser Service
Sep 09, 2025 ASTM-B338-Titanium.pdf
Why Grade 7 for Heat Exchanger and Condenser Tubes
Most titanium heat exchanger tube is Grade 2, and for oxidising service that remains the right answer. Grade 7 titanium, UNS R52400, is specified when the tube surface cannot stay clean. It is unalloyed titanium with 0.12% to 0.25% palladium, and the palladium changes the electrochemical behaviour of the surface so that the passive film survives in reducing media and in high-chloride environments at temperature.
The practical case for Grade 7 is almost always localised corrosion rather than uniform wastage. Crevices form under tube-to-tubesheet joints, support plates, gaskets and sludge deposits, and in those shielded sites the local chemistry turns acidic and oxygen-starved. Grade 2 fails there while a Grade 7 tube continues to perform, even though both grades would look identical on a flat coupon exposed to the bulk fluid.
Composition and Minimum Mechanical Properties
| Element | Limit (wt%) |
|---|---|
| Pd | 0.12 to 0.25 |
| C | 0.08 max |
| N | 0.03 max |
| O | 0.25 max |
| H | 0.015 max |
| Fe | 0.30 max |
| Ti | Balance |
| Property | Minimum, annealed |
|---|---|
| Tensile strength | 345 MPa (50 ksi) |
| Yield strength, 0.2% offset | 275 MPa (40 ksi) |
| Elongation in 50 mm | 20% |
| Density | 4.51 g/cm3 |
| Modulus of elasticity | 105 to 110 GPa |
Grade 7 is supplied as seamless or welded and annealed tube to ASTM B338, or as pipe to ASTM B861 and B862, with ASME equivalents SB338, SB861 and SB862 for coded pressure equipment. The withdrawn ASTM B337 designation should not be used on new orders.
Where Grade 7 Outperforms Grade 2
Reducing acids. In boiling dilute sulphuric acid, Grade 2 corrodes at a rate measured in millimetres per year while Grade 7 stays typically one to two orders of magnitude lower, often below 0.1 mm/y.
Hydrochloric acid service. Dilute hydrochloric acid attacks Grade 2 severely; the palladium addition extends the useful concentration and temperature range considerably, although each duty must still be checked against measured data.
Hot chloride brines. Grade 7 raises the temperature at which crevice attack starts in chloride solutions, which is what allows higher cooling water temperatures or less frequent cleaning.
Organic acid streams. Formic, acetic and oxalic acid media behave far better with the Pd-modified surface than with Grade 2.
Grade 7 does not help against fluoride ions, and it does not change the hydriding or dry chlorine hazards. Those are chemistry-specific limits that apply to all unalloyed titanium grades.
Tube Selection, Wall Thickness and Sizing
Tube selection starts with the U-value target and the pressure rating, then moves to the corrosive case:
Typical sizes are 19.05 mm, 25.4 mm and 31.75 mm outside diameter, with walls of 0.7 mm to 1.5 mm for condensers and exchangers.
Wall thickness must cover pressure, plus an erosion allowance for the shell-side fluid and a corrosion allowance if the environment is not fully benign.
U-bend radius should be at least two to three times the outside diameter for thin walls, and the bend must remain within the ductility of the annealed tube.
Order the annealed condition and state the test package: eddy current, hydrostatic proof, or ultrasonic inspection as the design requires.
A partial upgrade is often economically sound. Grade 7 tubes with a Grade 2 shell, or the reverse, can be justified where only one side of the exchanger sees the aggressive fluid, but the tubesheet material and the joint protection usually dominate the outcome, so the whole wet-side circuit should be reviewed together.
Welding, Expansion and Installation Practice
Weld tubes to tubesheets under full inert shielding. Weld colour is the acceptance criterion: bright silver is acceptable, any blue or grey tint means contamination.
Roller expand with controlled torque or a calibrated expander. Over-rolling raises residual stresses and can crack thin walls, while under-rolling leaves a leak path and a crevice.
Keep the joint clean. Grease, marking ink and chloride-bearing fluids trapped in the crevice defeat the corrosion resistance of the alloy itself.
Support the tube bundle so that vibration does not fret the tubes at baffles; fretting damage creates both a mechanical defect and a fresh crevice.
Store and handle tubes away from carbon steel surfaces, and rinse any pickling residue completely before service.
Typical Misapplications
Buying Grade 7 for an oxidising duty such as nitric acid or clean aerated seawater where Grade 2 is already immune, thereby paying a large premium for no benefit.
Using Grade 2 tube in a heavily fouling chloride stream and then blaming the grade when crevice corrosion appears at the tubesheet.
Assuming palladium protects against fluoride or dry chlorine, both of which attack all unalloyed titanium grades.
Overlooking the temperature ceiling. Design codes limit unalloyed titanium pressure service to roughly 315 C, and creep and oxidation, not corrosion, take over above that point.
Specifying the alloy but neglecting fabrication cleanliness, which reintroduces iron contamination and chloride residues at the very joints the alloy was bought to protect.
FAQ
Q: What is Grade 7 titanium tube used for?
Heat exchanger, condenser and chemical process tubes in reducing acids, mixed organic streams and hot chloride brines, where crevice corrosion at joints and deposits is the design concern.
Q: How much palladium does Grade 7 contain?
Between 0.12% and 0.25% by weight, balance titanium with controlled interstitial elements.
Q: Is Grade 7 stronger than Grade 2?
No. Both have a minimum tensile strength of 345 MPa and a minimum yield strength of 275 MPa in the annealed condition. Mechanical properties are essentially identical.
Q: Which ASTM standard covers Grade 7 heat exchanger tube?
ASTM B338 for seamless or welded tube, with ASME SB338 for coded pressure service. Pipe forms are covered by ASTM B861 and B862.
Q: Can Grade 7 tubes be welded to a Grade 2 tubesheet?
Yes, the joint welds normally with the same practice. The corrosion performance at the joint is then governed by the less resistant of the two components.
Q: Does Grade 7 tube need special cleaning before service?
It needs the same cleanliness as any titanium: no chloride residues, no embedded iron, and a fully rinsed surface after any acid pickling operation.